Time to dry 2-, 30, and 40inch S4S southern pine at 240°F, as related to board width

Informally Refereed
Download (PDF 1.77 MB): https://research.fs.usda.gov/download/treesearch/24183.pdf

Abstract

With 80°F wet-bulb depression and air cross-circulated at 1,000 fbm, southern pine in 2-, 3-, and 4-inch thicknesses attained 10 percent moisture content in 22.4, 35.6, and 45.3 hours. In 3- and 4-inch thicknesses, 4-inch-wide lumber required less time to dry than that 8 or 12 inches wide. Surface checks were absent or moderate in all thicknesses and widths. End-checking, absent or minor in 2-inch lumber, was moderate to severe in 3- and 4-inch lumber. At 10 percent moisture content, end checks in the thicker lumber were several inches long. Shrinkage and warp were within acceptable limits, and casehardening was relieved by 3 or 4 hours of conditioning.

Citation

Koch, Peter. 1973. Time to dry 2-, 30, and 40inch S4S southern pine at 240°F, as related to board width. Forest Products Journal, Vol. 24(3): 35-39